The National Institute of Advanced Industrial Science and Technology (AIST) and DOWA Holdings (DOWA) announced on November 18, 2026 that they have jointly developed a new coating device that can rapidly form metal films on the surface of powders. High-speed vacuum evaporation has traditionally been used mainly to coat flat substrates, and applying it to powders has been difficult. Powder being stirred in a container has to be supplied with metal vapor from above, but it was hard to hold heated, molten metal while releasing only the vapor downward. The two organizations devised a "deposit-down evaporation source" that reverses the flow of vapor with a dome-shaped crucible, and confirmed in zinc deposition on alumina powder that it far outperforms conventional sputtering in efficiency.

AD

Challenges specific to powder coating, unlike flat substrates

Powders used in battery materials, electronic components, catalysts and other applications can gain functions such as corrosion resistance, electrical conductivity and thermal conductivity when a thin metal film is formed on their surface. However, it is hard to form a film on powder using the same methods as for plate-like substrates. If film material is supplied to powder in a container from the side or from below, the container blocks it, and tilting or inverting the container would spill the contents. The metal therefore has to be supplied from above the open container, with the powder stirred as the film is formed.

The conventional technology that meets this condition is sputtering, in which ions strike a solid metal target in a vacuum, knocking out atoms that form the film. Because sputtering can supply metal atoms from top to bottom, it can be applied to powders, but its deposition rate is slow, so processing large quantities of powder with its large surface area takes time and money. Vacuum evaporation, which heats and vaporizes metal, is suited to fast deposition, but in its conventional structure the molten metal has to be held in a crucible, and the metal vapor was released mainly upward.

The new development aims to remove these constraints of vacuum evaporation and bring high-speed deposition to powders. The results are based on laboratory materials-processing tests using alumina powder and zinc, and no peer-reviewed paper or preprint on the device has been identified so far. Details are scheduled to be reported on the second day of the Society of Powder Technology, Japan 2026 Autumn Research Meeting, held November 24–25.

A dome-shaped crucible ejects metal vapor downward

The development team devised a dome-shaped crucible with an opening at the bottom. With no openings in the sides or top, heating the whole crucible in a high vacuum melts the metal inside and generates vapor from the liquid surface. According to AIST, when the rising metal vapor reaches the inner wall of the dome, which is kept hot, it changes direction without condensing and sticking, and is finally ejected downward through the opening at the bottom. This makes it possible to keep the molten metal inside while supplying only the vapor downward.

However, simply installing the evaporation source at the top of the vacuum chamber does not coat the powder surface uniformly. If the powder is stationary, only the upper layer of particles is exposed to the vapor, and metal hardly reaches the areas where particles touch one another. The lower part of the device therefore holds a mechanism combining a rotating disc-shaped container with a stirring jig. By rotating the container and stirring the contents, the orientation and position of the particles are constantly swapped, so that metal vapor reaches more particle surfaces.

Behind the development lies earlier joint research by AIST and DOWA on improving the heat resistance of magnetic powders. The two had developed a technology that forms a protective film on powder surfaces to suppress oxidative decomposition at high temperatures (JP 2025-48790). Industrializing it required a major increase in deposition speed, which led to the development of this evaporation device.

AD

Performance confirmed in zinc deposition on 200 g of alumina powder

The performance tests used 200 g of alumina powder, a type of ceramic, and 7.5 g of metallic zinc pellets. The alumina powder has a median particle size of 15.4 μm and a specific surface area of 2,248.36 cm²/g. Zinc was placed in an alumina crucible, and the vacuum chamber was evacuated to or below. While the powder was stirred, the evaporation source was heated to 750°C over 25 minutes and held at that temperature for 5 minutes. Zinc melts at about 420°C, so the test heated it to a temperature at which evaporation proceeds sufficiently.

Examination of the treated powder with a scanning electron microscope (SEM) and energy-dispersive X-ray spectroscopy (EDS) confirmed that a zinc layer had formed around the outside of the alumina particles. The average zinc content of the powder reached 3.2% by mass, and the team estimates the average film thickness at 20.6 nm. These results confirm that zinc vapor released downward reaches the surfaces of the stirred particles and can form a metal film.

However, the announcement does not give the number of test repetitions, the error range of the measurements, or the film-thickness distribution by particle. The evaluation also focused on the amount of zinc deposited and its distribution in particle cross-sections, and no measurement results have been published showing how much corrosion resistance, electrical conductivity, thermal conductivity, catalytic activity or post-sintering material properties actually improved.

Over 100 times the deposition efficiency of sputtering, with caveats on the corrected value

The team also ran a comparison test between the new device and conventional sputtering. For sputtering, a 2-inch-diameter zinc plate was used as the target, and zinc was deposited on alumina powder while argon gas was introduced. Average power consumption during steady operation was estimated at about 680 W for the new device and about 780 W for sputtering, so there was no large difference in power consumption itself.

The amount of zinc deposited per hour, however, differed by about 100 times. The new device recorded a measured 14.8 g/h, while sputtering reached 0.15 g/h after correction for differences in equipment conditions. Per unit of electrical energy, the new device achieved against for sputtering, showing about 113 times the deposition efficiency.

Deposition method Film material and powder Estimated average power consumption (W) Zinc deposited (g/h) Deposit per unit energy (g/Wh) Measured/corrected
Newly developed evaporation device Zinc / alumina powder About 680 14.8 Deposit measured; power estimated
Sputtering 2-inch zinc plate / alumina powder About 780 0.15 4x correction applied to measured 0.0376 g/h

What matters in this comparison is that the sputtering figure of 0.15 g/h is not a direct measurement. The zinc that actually adhered to the powder in the comparison test was 0.0376 g/h. However, the sputtering setup used a small container for small lots, and zinc that scattered outside the container also had to be taken into account. The team therefore multiplied the measured value by four, assuming the scattered material could have been used for deposition, and used that as the basis for comparison.

AIST explains that because a sputtering source has some directivity, the range over which material actually scatters and adheres is smaller than the range assumed in this correction. The 0.15 g/h figure is therefore a generous estimate in sputtering's favor. Even so, the new device's energy efficiency came out more than 100 times higher. Note, however, that this figure compares the equipment and test conditions used here and does not indicate a general performance gap against all sputtering systems.

AD

A simple configuration aimed at industrialization, with other metals under consideration

The structure is also expected to offer an advantage in material utilization. In sputtering and electron-beam evaporation, only part of the target material is used for deposition, and unused material remains after use. The new device, by contrast, vaporizes the metal feedstock in the crucible and uses it for deposition, which may reduce waste. However, no measured material utilization rate for this test has been published.

The relatively simple configuration is another feature. The main mechanisms are the dome-shaped crucible, its heater and the powder-stirring mechanism, and the device needs neither the circulating cooling water nor the process gases such as argon that sputtering uses. AIST believes this structure suits scaling up the equipment and increasing throughput. Combining multiple evaporation sources could also allow the formation of alloy or multi-component coating layers, not just single metals.

On the other hand, metals that evaporate less readily require higher heating temperatures, and choosing a suitable crucible material that does not react with molten metal at high temperatures is essential. The team aims next to develop a technology that deposits films directly onto clean surfaces before oxide films form, by keeping powder out of contact with air before and after coating, and to extend the approach to powders that react readily.

At the Society of Powder Technology, Japan 2026 Autumn Research Meeting on November 25, 2026, AIST's Wataru Yamaguchi and Yusuke Hirayama, and DOWA's Yoshiyuki Domyo, Yasuhito Miyamoto, Tomoya Yamada and Tetsuro Tokumoto are scheduled to present details under the title "Powder Coating Device Using a Deposit-Down Evaporation Source."